Weld Blog

Materials

Metals for beginner welders

Each metal reacts to heat in its own way. Some flow easily, some crack, some warp and some hide a coating that needs to come off first. Knowing what you are welding sets the process, the filler and the prep.

Mild steel

Low-carbon (mild) steel is where nearly everyone starts. It is cheap, easy to find as plate, tube and angle, and it welds well with every process covered here. Its melting range is roughly 1,400 to 1,500°C (about 2,600 to 2,800°F), and the puddle is easy to see and control.

New hot-rolled steel carries a dark blue-gray skin of mill scale. Grind or brush it off where the weld and the work clamp go. Cold-rolled steel has a smoother, cleaner surface. Rust, paint and oil also need to come off. Clean metal is the single biggest help to a beginner's welds.

Stainless steel

Stainless steel contains chromium, which gives it a protective surface layer. It holds heat in the weld area longer than mild steel, so it warps more easily and can discolor. Use lower heat, keep beads short and let the part cool between passes. Match the filler to the type of stainless, which the filler package lists.

The colors around a stainless weld, from straw to blue, show how hot the surface got. The weld bead swatch for TIG on the home page draws that tint. Fumes from stainless can contain hexavalent chromium, so use local exhaust. See ventilation and fire safety.

Aluminum

Aluminum is light and common, and it is harder to weld for three reasons:

  • It conducts heat away quickly, so the joint needs more heat to start and then less as the part warms up.
  • Its surface oxide melts at a far higher temperature than the metal under it, above 2,000°C against about 660°C. The oxide has to be cleaned off and broken up during welding.
  • It does not change color before it melts, so it can slump with little warning.

Aluminum is usually welded with TIG on AC, or with MIG using pure argon and a setup that handles soft aluminum wire. Clean it with a stainless brush kept only for aluminum, and weld soon after cleaning.

Cast iron

Cast iron has a high carbon content and tends to crack as it cools. Repairs often use preheating, special filler rods, short beads and slow cooling. It is not a beginner material. Practice on steel first and research the specific casting before you try.

Coated and unknown metals

Galvanized steel has a zinc coating that gives off harmful fumes when heated, so grind it away from the weld zone and ventilate well. Painted and plated parts need stripping. If you do not know what a scrap piece is made of, a magnet helps: mild steel and most cast iron stick, aluminum and many common stainless grades do not. When unsure, do not weld it for anything that carries a load.

Thickness and heat

Thin metal needs less heat and faster travel, or it burns through. Thick metal needs more heat, sometimes beveled edges and several passes to fuse all the way through. Your machine's chart pairs metal thickness with starting settings. Practice on scrap of the same thickness as your project.

MetalGood first processMain challenge
Mild steelMIG, flux-core or stickClean off mill scale and rust
Stainless steelTIG or MIGHeat control and warping
AluminumTIG on AC, or MIG with argonOxide layer and fast heat loss
Cast ironStick with special rodsCracking as it cools

Once you know the metal, choose the joint: see weld joints and positions.

Metal questions

Can I weld steel to aluminum?

Not with ordinary arc welding. They do not mix well in a weld puddle. Joining them takes special methods or mechanical fasteners.

Why does my steel warp after welding?

Weld metal shrinks as it cools and pulls the parts with it. Tack the parts first, alternate sides, keep beads short and clamp the work to reduce it.