Weld Blog

Process ยท SMAW

Stick welding explained

Stick welding uses a metal rod coated in flux, held in a clamp. The rod is both the electrode and the filler, and its coating makes the shield. The gear is simple and it works on dirty steel and in the wind.

What melts in
Flux-coated rod held in a clamp
Shielding
The coating burns into gas and slag
Current
AC or DC, depending on the rod
Slag
Heavy layer to chip off
In wind
Good: the coating makes its own shield

How stick works

A stick setup has a power source, an electrode holder (the stinger), a work clamp and a box of rods. You strike an arc between the rod and the work, and the rod's metal core melts into the joint. The coating burns to make shielding gas and melts into slag that floats on top of the weld. The formal name is shielded metal arc welding, or SMAW.

As the rod burns down, you feed it toward the work to keep the arc length steady. When it gets short, you stop, chip, and put in a new rod.

Reading a rod number

Steel rods for this kind of work carry a code like E6013 or E7018. The parts mean:

PartExampleMeaning
EE7018Electrode
First two digits70Minimum tensile strength of the weld metal in thousands of psi (70,000 psi)
Third digit1Positions: 1 means all positions, 2 means flat and horizontal only
Last digit8Read with the third digit: coating type and which current it runs on

A few common types: E6010 and E6011 dig in deeply and burn through some rust. E6013 runs smoothly with an easy-to-remove slag and suits light work. E7018 is a low-hydrogen rod used for structural steel. It needs to be kept dry, and shops store it in a rod oven once the package is open. The rod box lists the current, polarity and amperage range.

Striking and holding the arc

  1. Set the amperage inside the range on the rod box. Thicker rods need more current.
  2. Strike the arc by scratching the rod tip across the metal like a match, or by tapping it, then lift slightly.
  3. Hold an arc length of about the diameter of the rod's metal core. Too long and the arc spatters and wanders. Too short and the rod sticks.
  4. Tilt the rod about 10 to 20 degrees back toward the finished weld and drag it along the joint.
  5. Feed the rod down steadily as it burns, and travel at a pace that keeps the bead even.

If the rod sticks, twist or snap it free, or let go of the stinger's grip and release it. Do not touch the rod with a bare hand while the machine is on.

AC and DC

Basic stick machines may supply AC only, DC only, or both. DC gives a smoother, steadier arc and works with a wider range of rods. Some rods are made to run on AC. Match the machine to the rod: the box tells you which currents and polarities it accepts.

Strengths and trade-offs

Stick handles rust, paint residue and mill scale better than the gas processes, keeps working in the wind, and the gear is compact. It suits thicker steel, repair work and outdoor jobs. The trade-offs: striking and holding an arc takes practice, thin sheet is easy to burn through, and every bead needs the slag chipped off before the next pass.

See how it compares on choosing a process, and set up your work area with ventilation and fire safety in mind.

Stick questions

Why does my rod keep sticking?

The usual causes are amperage set too low, an arc held too short, or a damp rod. Turn the amperage up within the range on the box, strike with a quick scratch, and lift a little faster.

Why is it called stick welding?